Eliane Farhi, doctorante dans l’équipe Physico-chimie et dynamique des surfaces.

Growth dynamics of Fe-bearing intermetallics in model Al-Si-Fe and Al-Si-Fe-Mn alloys: in situ observations

Résumé

Le recyclage de l’aluminium impose de tolérer des teneurs croissantes en fer, impureté qui précipite lors de la solidification sous forme de phases intermétalliques riches en cet élément, dont la morphologie facettée dégrade les propriétés de l’alliage. Le manganèse est couramment ajouté pour substituer à la phase β-Al₅FeSi, en plaquettes, la phase α-Al₁₅(Fe, Mn)₃Si₂ (α-IM), moins néfaste. Les mécanismes de germination et de croissance de ces phases facettées, et la formation de microstructures eutectiques irrégulières restent toutefois mal compris.

La présente étude est faite par microscopie optique in situ lors de la solidification dirigée d’alliages à base Al–Si–Fe(–Mn) en échantillons minces. Nous avons développé un dispositif d’observation original à deux échelles combinant des optiques à champs de vision macroscopique (MFOV) et microscopique (µFOV). En complément, des analyses chimiques et cristallographiques ex situ ont été faites sous microscope électronique. Trois systèmes de complexité croissante sont examinés.

  1. Dans l’eutectique ternaire Al–Si–Fe, la croissance triphasée (FCC-Al + Si + β-IM) est irrégulière, mais devient d’autant plus couplée que la vitesse de tirage augmente. Les deux phases facettées présentent de nombreuses macles.
  2. Dans l’alliage quaternaire Al–Si–Fe–Mn, la transition « facetté vers branché » des cristaux α-IM est identifiée comme le passage d’une croissance facettée quasi libre à un couplage eutectique biphasé avec FCC-Al, formant deux populations de colonies primaires et secondaires. Nous analysons le poids respectif des interactions par diffusion solutale et de la cinétique interfaciale dans la dynamique de croissance.
  3. L’ajout de baryum et de cobalt dans ce même alliage produisent des effets opposés : le baryum supprime le couplage primaire et disperse la taille des colonies, tandis que le cobalt augmente la densité de germination et affine la microstructure.

En reliant systématiquement chaque écart à un état quasi-stationnaire de référence, ce travail porte une analyse cohérente depuis un eutectique ternaire jusqu’à des microstructures multi-composants et multi-populations d’intérêt industriel.

Abstract

Recycling aluminium requires tolerating increasing iron contents. This impurity precipitates during solidification in the form of iron-rich intermetallic phases, whose faceted morphology compromises the properties of the alloy. Manganese is commonly added in order to replace the plate-like β-Al₅FeSi phase with the less detrimental α-Al₁₅(Fe, Mn)₃Si₂ phase (α-IM). The nucleation and growth mechanisms of these faceted phases, as well as the formation of irregular eutectic microstructures, nevertheless remain poorly understood.

The present study is carried out by in situ optical microscopy during the directional solidification of Al–Si–Fe(–Mn) based alloys in thin samples. We have developed an original two-scale observation set-up combining macroscopic (MFOV) and microscopic (µFOV) field-of-view optics. In addition, ex situ chemical and crystallographic analyses were performed under an electron microscope. Three systems of increasing complexity are examined.

  1. In the Al–Si–Fe ternary eutectic, three-phase growth (FCC-Al + Si + β-IM) is irregular, but becomes increasingly coupled as the pulling velocity increases. Both faceted phases exhibit twinning.
  2. In the Al–Si–Fe–Mn quaternary alloy, the “faceted to branched” transition of the α-IM crystals is identified as the change from quasi-free faceted growth to two-phase eutectic coupling with FCC-Al, forming two populations of primary and secondary colonies. We analyse the respective weight of solutal diffusion interactions and of interfacial kinetics in the growth dynamics.
  3. The addition of barium and of cobalt to this same alloy produces opposite effects: barium suppresses primary coupling and disperses the colony size, whereas cobalt increases the nucleation density and refines the microstructure.

By systematically relating each departure to a reference quasi-steady state, this work provides a consistent analysis ranging from a ternary eutectic to multi-component, multi-population microstructures of industrial interest.

 

Jury

  • Silvère AKAMATSU (Directeur de recherche – INSP) Co-Directeur de thèse
  • Sabine BOTTIN-ROUSSEAU (Professeur – INSP) Co-Directrice de thèse
  • Patrick S. GRANT (Professeur – University of Oxford) Rapporteur
  • Ulrike HECHT (Ingénieur – Access e.v.) Examinatrice
  • Nathalie MANGELINCK-NOEL (Directrice de recherche – IM2NP) Rapportrice
  • Mehdi MEDJKOUNE (Maître de Conférence – IJL) Invité
  • Mathis PLAPP (Directeur de recherche – LPMC) Examinateur